Author Topic: Charlies Angels Restoration  (Read 8650 times)

0 Members and 7 Guests are viewing this topic.

Offline Brettski

  • Trade Count: (0)
  • *****
  • Forum Posts:
  • Gold Coast, Queensland
  • Since I Was A Young Boy I Played The Silver Ball!
    • Strikes and Spares Restoration
Re: Re: Charlies Angels Restoration
« Reply #45 on: May 21, 2016, 11:26:32 PM »
Nice good to see the plating kits in action I'll get one one day

Hey Gav, this is a home brew kit

I had the power supply already but the rest cost about $30 - $40 I also bought gloves for using the Acid which you use to clean it with prior to electroplating

Bucket - Bunnings
Copper Wire (stripped it out of some scrap inner wall power cable)
Thin copper wire for hooks
Hydroclauric Acid - Bunnings
6 litres White Vinegar - Aldi (cheap)
1 kg Epsom salts
1 kg white sugar
Zinc Anodes - (free from local electroplating place)

If anyone is interested I can post the process, the results are fantastic once polished. I will post some pics tomorrow.

Brettski... :)
Project is looking great mate. Would definitely be interested in more info on your home brew plating!

Sent from my SM-G930F using Tapatalk

Here is the recipe and method I use for my Zinc Plating..

Home Zinc Plating Instructions..
 

9 - 11 Litre plastic bucket

Zinc anodes... I got a handfull of zinc balls from a local elecrtroplater.

1kg of Epsom salts

6 - 8 litres of white vinegar...Aldi $1.19 ltr

1.5kg of white sugar to be used as a brightener.

Thick copper wire for the anodes, I used some stripped back inner wall electrical cable.

A few strands of light guage copper wire for hanging parts.

1 piece of copper water pipe or use the thick copper wire cable tied to a piece of wood for the cathode hanger

Multi Power Supply, I have one that has 2v, 4v, 6v, 8v, 10v, 12v, I only use the two volts mostly and for bigger parts 4v (slower adhesion at lower voltages but better quality)

200ml of hydrochloric acid to be used as an acid dip before plating... you can get this at Bunnings.

Fine grade steel wool.

 

Method

Electrolyte

Mix Vinegar, Epsom salts and sugar together until dissolved in the bucket.

Drill a small hole in two zinc balls, then attach reasonable lengths of the heavier gauge copper wire to them with screws and place them in the bucket at equal spacing, do not let the screws touch the water then bend the wire over the edge of the bucket to support them in place and wire them in such a way that they are both connected and there is some bare wire to connect your power to. (See pic)


Next get your copper pipe and flatten the ends the same width as the bucket so it doesn't roll and while doing this squash a piece of heavy gauge wire in one end... this will be your cathode hanger. Or use thick copper wire cable tied to a piece of wood.

Place this on top of the bucket and make sure it is not touching any of your anode wiring or it will short out.

Attach the positive to the anode (Zinc) wiring and the negative to the cathode wire (copper pipe).... turn on power and your almost ready to start.

Now before plating your good parts you need to plate out the electrolyte... this sets up the solution for complete surface coating.... this means you have to get zinc ions in the solution for it to plate quickly and evenly.

To do this you need roughly a square piece of metal about 50mm square that has been wire brushed of all contaminates and dipped in the hydrochloric solution (read about hydrochloric solution below) and hang this submerged in your electrolyte with the power on. You should see a slight fizzing going on....this needs to run like this overnight if possible. I also placed an extra zinc ball into the water which just sat on the bottom during this process.

 

Hydrochloric solution.

1 litre of water to 200ml of acid mixed well.....wear gloves and glasses as this stuff burns like nothing else so be very carefull.

This will be your parts dip..... keep another bucket of plain water handy to rinse parts after dipping.

 

Parts cleaning and plating

Clean all dirt and grease of the parts before doing anything else, I use dish washing detergent and water.

Then hang your parts in the hydrochloric solution... you may see some fizzing going on, this will be the previous zinc coating being dissolved by the acid and this will also remove surface rust.

After the fizzing has stopped rinse the part thoroughly in fresh water and dry off with a rag.

Next you need to wire wheel the part back to bright steel.

Once that is done dip your part into the hydrochloric acid quickly and then rinse and very quickly hang in the zinc bucket submerged, if you wait to long to hang it, it will flash rust and you will have to start again.

Now that it is in the zinc bucket you can leave it to do it's thing, you will see some fizzing and that's good, it is now being plated with zinc. Leave it in the zinc bucket for 30  minutes or until completely plated evenly

When you pull the part out it will have a dull grey appearance but should be completely coated in zinc.

 

Brightening up the part.


You can clean the part up with some fine grade steel wool or buff it on a polishing wheel to get a chrome like appearance.

You can also use a week solution of aluminium cleaner (chemtech BLITZ) available at Supercheap mixed with water.

Dip your parts in this one at a time and using a stainless parts cleaning brush brush the parts to a bright shine then finish of with fine steel wool.... when satisfied rinse off with water and dry. ( wear gloves and glasses when doing this.)

You can replate at this stage if you want a heavier coating of zinc then repeat the cleaning procedure.

The attached picture should help with the instructions.

Hope this helps..

Cheers: Brettski... :)